ON-DEMAND OPEN DATABASES · fetch_material & search_remote_materials

Open Materials & Constitutive Library

Pull validated constitutive data directly from refractiveindex.info, AFLOW, Materials Project, and NumBAT into unit-explicit TOML, or extend 42 bundled baseline files.

OPEN MATERIAL REPOSITORIES

Fetch validated material data from public repositories

The bundled library below is an offline starting point. Using fetch_material, search_remote_materials, list_remote_materials, and import_material, nyx retrieves entries over HTTPS from refractiveindex.info, AFLOW, the Materials Project, and NumBAT, checks units and stability, and writes TOML records that inherit from bundled baselines via extends.

CLI & ENGINE · FETCH & SEARCH PUBLIC DATABASES
# Fetch curated or live entries and extend a bundled baseline cleanly
nyx material fetch rii main/Si/nk/Green-2008 --extends silicon --name silicon_green --save

# Or from Monty scripts / MCP commands:
search_remote_materials(query="LiNbO3", source="all", live=true)
fetch_material(source="rii:main/SiO2/Malitson", name="fused_silica_ref", add_to_project=true)

Every material in nyx — whether fetched on demand from a public repository or loaded from the local library — compiles into a plain-text TOML file (format = 2, validated against docs/architecture/contracts/material_schema.v2.json) where every physical quantity carries an explicit unit (“496.8 GPa”, “2500 kg/m^3”, “1395 ueV”). Missing units, positive-definiteness violations, or wavelengths evaluated outside a formula’s declared range = [min, max] are rejected immediately with the exact table and key name — silent extrapolation is not permitted.

Constitutive Sections & Crystallography

  • [elastic]: Isotropic (E, nu, lambda, mu, or K, G), symmetry-class (isotropic, cubic, hexagonal, trigonal, tetragonal, orthotropic, monoclinic, triclinic), full 6×6 stiffness matrix, or compliance matrix in textbook Voigt order 1=xx, 2=yy, 3=zz, 4=yz, 5=xz, 6=xy with engineering shear strain. Crystal regions are rotated into the wafer frame by Bunge Z-X-Z intrinsic Euler angles.
  • [optical]: Supports constant, sellmeier, cauchy, tabulated (monotone cubic pchip or linear), schott, herzberger, rii_formula_4, rii_formula_5, rii_formula_6, drude, lorentz, and drude_lorentz, plus linear dn_dT, cryogenic Bose–Einstein dn_dT_model, uniaxial ([optical.ordinary] / [optical.extraordinary]), and biaxial (x/y/z) dispersion.
  • [thermal] & [electrical]: Scalar, diagonal, 6-component, or { perp, par } tensors with continuous temperature curves (tabulated_T, NIST log10_poly, or einstein_shift).
  • Microwave & Quantum ([dielectric], [superconducting], [interfaces.{ma,ms,sa}]): Complex microwave permittivity $\tilde{\varepsilon}_r(T) = \varepsilon_r(1 - i \tan\delta(T))$ with optional TLS saturation (tls_tan_delta_0, tls_E_c, tls_T_0, tls_beta), oxide interface participation thickness and loss tangent, and Mattis–Bardeen superconducting thin-film parameters (tc, gap_0, lambda_L, xi_0, sigma_n, dynes_gamma, r_res, nominal_thickness).
  • Coupled Tensors: Full crystal-frame [piezoelectric] (e in C/m^2 or d in pC/N with thermodynamic check $C^D - C^E = e^T (\varepsilon^S)^{-1} e$), [photoelastic] ($p_{IJ}$), [electro_optic] ($r_{IJ}$), and positive semi-definite [viscoelastic] dynamic viscosity $\eta_{IJ}$ for Akhiezer/Kelvin–Voigt $Q_m$ damping.

Inheritance (extends) & Provenance

Every table carries a source citation and optional verified date; unverified estimates must carry "APPROXIMATE" or "UNVERIFIED". Custom or measured materials inherit cleanly via extends = "silicon" without duplicating tensors: each overridden table replaces its parent table atomically so units and parameters never mix across sources.

Bundled Domains & CLI Evaluator

The shipped library spans five domains — base optical/RF/thermal (air, aluminium, copper, gold, lithium_niobate, silica, silicon, silicon_nitride, silver), photonics author/process variants (silicon_salzberg, silicon_palik, silicon_nitride_philipp, silicon_nitride_pecvd, lithium_niobate_mgo, gallium_arsenide, gallium_arsenide_papatryfonos, gold_johnson, silver_johnson), phononics, crystals & MEMS (silicon_mcskimin, silica_thermal_box, quartz_alpha, polysilicon_polymumps, aluminum_nitride, aluminum_nitride_piezomumps, scaln_30, diamond), cryogenic 4 K baselines (silicon_4k, silica_4k, lithium_niobate_4k, copper_4k), and superconducting films (aluminium_sc_emft, niobium_sc, titanium_nitride_sc, niobium_titanium_nitride_sc, granular_aluminium_sc, nbn_sc, beta_tin_sc).

nyx material list
nyx material show niobium_sc
nyx material eval niobium_sc --temp 0.02 --freq 5e9 --thickness 100e-9
nyx material bcs niobium_sc --freq 5e9 --temp 0.02 --thickness 100e-9
nyx material fetch rii main/Si/nk/Green-2008 --extends silicon --name silicon_green --save
BUNDLED BASELINES · materials/*.toml

Bundled Baseline Records (42 Public TOML Files)

42 / 42
Material Kind Point Group Tref / ρ Capabilities Description & Provenance
air fluid isotropic
300 K
1.2 kg/m^3
thermalelectricaloptical
Dry air idealized optically as vacuum (n = 1.0, eps_r = 1.0, rho = 1.2 kg/m^3 at 300 K) — lossless background cladding baseline.
Compiled from the per-table sources below. Density 1.2 kg/m^3 is the usual room-temperature figure: APPROXIMATE, not checked against a reference in this library
aluminium metal isotropic
293.15 K
2700 kg/m^3
elasticthermalelectricalopticalsuperconducting
Evaporated/MEMS aluminium at 293 K (Rakic 1998 Lorentz-Drude 0.06-248 um; E=70 GPa, k=237 W/(m*K)) — room-temperature normal-metal/electrode baseline vs mK superconducting aluminium_sc_emft.
APPROXIMATE bulk/MEMS aluminium mechanics/thermal/electrical at 293 K + verified Rakic et al. 1998 [optical] fit (0.062-248 um)
aluminium_sc_emft superconductor isotropic
0.01 K
2700 kg/m^3
elasticthermalelectricalopticalsuperconductinginterfaces
Evaporated 150 nm Al superconducting film on FZ-Si at <1 K (standard_die.materials.AL: Tc=1.20 K, lambda_L=70 nm, Lk=0.20 pH/sq, E=77.5 GPa) — Josephson junction and mK CPW film vs 293 K aluminium.
APPROXIMATE thin-film cryogenic Al compilation from standard_die.materials.AL & McRae et al., Rev. Sci. Instrum. 91, 091101 (2020) + Kamm & Alers 1964 4.2 K Al mechanics
aluminum_nitride crystalline 6mm
293.15 K
3260 kg/m^3
elasticthermaldielectricopticalpiezoelectricphotoelasticelectro_opticviscoelastic
Single-crystal wurtzite AlN (Tsubouchi 1985 hexagonal c33=389 GPa + Pastrnak 1966 uniaxial Sellmeier 0.22-5.0 um, no=2.119 at 1.55 um) — bulk/epitaxial piezo-optomechanics benchmark vs sputtered aluminum_nitride_piezomumps and scaln_30.
K. Tsubouchi and N. Mikoshiba, Zero-temperature-coefficient SAW delay line on AlN epitaxial films, IEEE Trans. Sonics Ultrason. SU-32, 634-644 (1985): density 3260 kg/m^3
aluminum_nitride_piezomumps polycrystalline 6mm
293.15 K
3260 kg/m^3
elasticthermaldielectricopticalpiezoelectric
Reactive-sputtered c-axis polycrystalline AlN thin film (MEMSCAP PiezoMUMPs E=330 GPa + Beliaev 2021 n=2.018 at 1.55 um) — softer foundry MEMS/waveguide film vs single-crystal aluminum_nitride and alloyed scaln_30.
APPROXIMATE sputtered AlN film mechanics/thermal/electrical from A. Cowen et al., PiezoMUMPs Design Handbook Rev. 1.3 (MEMSCAP Inc.)
beta_tin_sc superconductor isotropic
1.5 K
7287 kg/m^3
elasticthermalsuperconducting
Clean Type-I superconducting beta-Sn (white tin) compared with Nb and Al for low-Tc BCS benchmarks and RF joints
APPROXIMATE representative beta-Sn superconducting and mechanical dataset (Kittel / Poole Handbook of Superconductivity)
copper metal isotropic
293.15 K
8960 kg/m^3
elasticthermalelectricaloptical
Copper at 293 K (Rakic 1998 Lorentz-Drude 0.21-12.4 um; E=130 GPa, k=401 W/(m*K), Cp=385 J/(kg*K)) — room-temperature normal-metal baseline vs RRR=100 cryogenic copper_4k.
APPROXIMATE bulk OFHC polycrystalline mechanics/thermal/electrical at 293 K + verified Rakic et al. 1998 [optical] fit (0.207-12.4 um)
copper_4k metal isotropic
4.0 K
8960 kg/m^3
elasticthermalelectricaloptical
Cryogenic OFHC copper (RRR=100) at 4 K (NIST Cryo DB k=642.3 W/(m*K), Cp=0.0994 J/(kg*K), Ledbetter 1974 E=138 GPa) — dilution-refrigerator thermalisation metal vs 293 K copper.
Cryogenic 4 K properties for OFHC copper (RRR = 100); [optical] inherited from Rakic 1998 copper
diamond crystalline m-3m
298.15 K
3515 kg/m^3
elasticthermaldielectricopticalphotoelasticviscoelastic
Single-crystal IIa/CVD diamond (McSkimin & Andreatch 1972 cubic c11=1076.4 GPa + Phillip & Taft 1964 UV-MIR table n=2.3878 at 1.55 um) — highest acoustic velocity (~17.5 km/s) and thermal conductivity (2200 W/(m*K)).
H. J. McSkimin and P. Andreatch Jr., Elastic moduli of diamond as a function of pressure and temperature, J. Appl. Phys. 43, 2944-2948 (1972): density 3515 kg/m^3
gallium_arsenide semiconductor -43m
295.15 K
5317 kg/m^3
elasticthermaldielectricopticalpiezoelectricphotoelasticelectro_optic
Undoped bulk GaAs cubic crystal (Blakemore 1982 elastic c11=118.8 GPa + Skauli 2003 IR Sellmeier 0.97-17 um, n=3.3702 at 1.55 um) — sub-bandgap III-V photonics/SAW baseline vs absorbing gallium_arsenide_papatryfonos.
J. S. Blakemore, Semiconducting and other major properties of gallium arsenide, J. Appl. Phys. 53, R123-R181 (1982): density 5317 kg/m^3 at 300 K
gallium_arsenide_papatryfonos semiconductor -43m
295.15 K
5317 kg/m^3
elasticthermaldielectricopticalpiezoelectricphotoelasticelectro_optic
MBE GaAs UV-SWIR complex n,k table (Papatryfonos 2021 ellipsometry, 0.26-1.88 um) — resolves the 870 nm direct-bandgap absorption edge unlike sub-bandgap lossless Skauli gallium_arsenide.
Mechanical, thermal and electrical properties inherited from gallium_arsenide; [optical] complex n,k ellipsometry from Papatryfonos et al. 2021 (refractiveindex.info main/GaAs/Papatryfonos, CC0)
gold metal isotropic
293.15 K
19300 kg/m^3
elasticthermalelectricaloptical
Evaporated Au wide-band Lorentz-Drude fit at 293 K (Rakic 1998, 0.25-6.2 um; E=78 GPa, sigma=4.52e7 S/m) — broadband analytical baseline vs lower-loss NIR experimental gold_johnson.
APPROXIMATE bulk polycrystalline mechanics/thermal/electrical + verified Rakic et al. 1998 [optical] fit (0.248-6.2 um)
gold_johnson metal isotropic
293.15 K
19300 kg/m^3
elasticthermalelectricaloptical
Evaporated Au thin-film experimental n,k table (Johnson & Christy 1972, 0.188-1.937 um) — lower intraband damping above 600 nm than Rakic 1998 Drude-Lorentz gold; standard visible/NIR plasmonics benchmark.
Mechanical, thermal and electrical properties inherited from gold; [optical] Johnson & Christy 1972 evaporated Au table (refractiveindex.info main/Au/Johnson, CC0)
granular_aluminium superconductor
2700 kg/m^3
superconducting
Granular aluminium (grAl) dirty-limit superinductor film (Maleeva 2018 / Gruenhaupt 2019: Tc=1.90 K, Delta_0=0.30 meV, sigma_n=2.5e4 S/m) — compact alias of granular_aluminium_sc.
Compiled from the per-table sources below (dirty-limit grAl film parameters from Maleeva et al. 2018 and Gruenhaupt et al. 2019)
granular_aluminium_sc superconductor isotropic
0.02 K
3000 kg/m^3
elasticthermalsuperconductinginterfaces
Nano-granular Al/AlOx superconducting superinductor film grAl (Grunhaupt 2019 / Maleeva 2018: Tc=1.8-2.1 K, Lk=200-2500 pH/sq) — high-impedance fluxonium superinductor vs clean low-Lk aluminium_sc_emft.
APPROXIMATE granular aluminum compilation from L. Grunhaupt et al., Nat. Mater. 18, 816-819 (2019) & N. Maleeva et al., Nat. Commun. 9, 3889 (2018)
graphene semiconductor 6/mmm
300 K
2267 kg/m^3
thermalelectricalsheet_2d
Monolayer graphene (2D zero-thickness Dirac semimetal sheet, Kubo intraband + interband conductivity)
L. A. Falkovsky and A. A. Varlamov, Space-time dispersion of graphene conductivity, Eur. Phys. J. B 56, 281-284 (2007)
lithium_niobate crystalline 3m
294.15 K
4640 kg/m^3
elasticthermaldielectricopticalpiezoelectricphotoelasticelectro_opticviscoelasticnonlinear
Congruent bulk/TFLN LiNbO3 at 294 K (Weis & Gaylord 1985 trigonal c11=203 GPa + Zelmon 1997 uniaxial Sellmeier 0.4-5 um, ne=2.1376 at 1.55 um) — undoped baseline vs photorefractive-resistant lithium_niobate_mgo and cryogenic lithium_niobate_4k.
R. S. Weis and T. K. Gaylord, Lithium niobate: Summary of physical properties and crystal structure, Appl. Phys. A 37, 191-203 (1985): density 4640 kg/m^3 (Kushibiki et al. 1999 SAW-grade Archimedes measurement is 4642.8 kg/m^3)
lithium_niobate_4k crystalline 3m
4.0 K
4640 kg/m^3
elasticthermaldielectricopticalpiezoelectricphotoelasticelectro_opticviscoelasticnonlinear
Cryogenic congruent LiNbO3 at 4 K (~2.5% stiffened trigonal C^E c33=248 GPa, clamped cryo eps=[44.3, 44.3, 26.5]) — mK piezo-optomechanical transducer model vs room-temperature lithium_niobate.
APPROXIMATE 4 K extrapolated thermoelastic stiffening and clamped microwave permittivity + inherited lithium_niobate density and Zelmon [optical]
lithium_niobate_mgo crystalline 3m
294.15 K
4640 kg/m^3
elasticthermaldielectricopticalpiezoelectricphotoelasticelectro_opticviscoelasticnonlinear
5 mol% MgO-doped congruent LiNbO3 uniaxial Sellmeier (Zelmon 1997, 0.4-5.0 um, ne=2.1299 at 1.55 um) — optical-damage-resistant nonlinear variant (lower ne than undoped congruent lithium_niobate).
Mechanical, thermal and electrical properties inherited from congruent lithium_niobate; [optical] from Zelmon et al. 1997 5 mol% MgO:LiNbO3 (refractiveindex.info MgO-LiNbO3, CC0)
nbn superconductor
8470 kg/m^3
superconducting
Niobium nitride (NbN) disordered superconducting thin film (Semenov 2009 / Wang 1996: Tc=14.5 K, Delta_0=2.40 meV, lambda_L=50 nm, xi_0=5 nm, sigma_n=5.0e5 S/m) — compact alias vs 16 K nbn_sc.
Compiled from the per-table sources below. Density 8470 kg/m^3 (APPROXIMATE stoichiometric delta-NbN density)
nbn_sc superconductor m-3m
4.0 K
8400 kg/m^3
elasticthermalsuperconductinginterfaces
High-kinetic-inductance B1 rocksalt NbN thin film compared with Nb and TiN for SNSPDs and compact resonators
APPROXIMATE representative sputtered delta-NbN thin-film superconducting RF dataset (Kamlapure 2010; Annunziata 2010)
niobium superconductor
8570 kg/m^3
superconducting
Niobium sputtered superconducting film (Park 2026 / Maxfield & McLean 1965: Tc=9.2 K, Delta_0=1.395 meV, lambda_L=33.3 nm, xi_0=39.0 nm, sigma_n=5.5e7 S/m) — compact BCS alias of niobium_sc.
Compiled from the per-table sources below. Density 8570 kg/m^3: C. Kittel, Introduction to Solid State Physics, 8th ed. (Wiley, 2005)
niobium_sc superconductor m-3m
4.2 K
8570 kg/m^3
elasticthermalopticalsuperconductinginterfaces
Nb superconducting film/crystal at 4.2 K (Carroll 1965 BCC c11=252.7 GPa + Golovashkin 1969 4.2 K n,k 0.4-9.2 um; Tc=9.2 K, lambda_L=90 nm, Lk=0.09 pH/sq) — highest elemental Tc for SFQ and cQED resonators.
K. J. Carroll, Elastic constants of niobium from 4.2 to 300 K, J. Appl. Phys. 36, 3689-3690 (1965): density 8570 kg/m^3
niobium_titanium_nitride_sc superconductor isotropic
4.0 K
7800 kg/m^3
elasticthermalsuperconducting
Disordered NbTiN superconducting thin film at 4 K (Samkharadze 2016: Tc=12.5-14.8 K, Bc2>10 T, Lk=3-40 pH/sq) — magnetic-field-resilient spin/hybrid cQED and TWPA film vs titanium_nitride_sc and niobium_sc.
APPROXIMATE disordered NbTiN film compilation from N. Samkharadze et al., Phys. Rev. Appl. 5, 044004 (2016)
polysilicon_polymumps polycrystalline isotropic
293.15 K
2330 kg/m^3
elasticthermaldielectric
LPCVD polycrystalline silicon structural film (MEMSCAP PolyMUMPs Rev. 13.0, E=158 GPa, nu=0.22, rho=2330 kg/m^3) — isotropic grain-averaged MEMS resonator film vs anisotropic single-crystal [100] silicon.
D. Koester, A. Cowen, R. Mahadevan, M. Stonefield, B. Hardy, PolyMUMPs Design Handbook Rev. 13.0 (MEMSCAP Inc.); Sharpe et al., JMEMS 1997 (APPROXIMATE grain-size-dependent polysilicon film properties)
quartz_alpha crystalline 32
293.15 K
2648.5 kg/m^3
elasticthermaldielectricopticalpiezoelectricphotoelastic
Single-crystal alpha-quartz SiO2 (Bechmann 1958 trigonal c11=86.74 GPa + Ghosh 1999 uniaxial Sellmeier 0.198-2.05 um, no=1.5277 at 1.55 um) — anisotropic piezoelectric SAW/BAW crystal vs amorphous fused silica.
R. Bechmann, Elastic and piezoelectric constants of alpha-quartz, Phys. Rev. 110, 1060-1061 (1958): density 2648.5 kg/m^3
scaln_30 crystalline 6mm
293.15 K
3380 kg/m^3
elasticthermaldielectricpiezoelectricelectro_optic
30% Sc-alloyed wurtzite Sc0.30Al0.70N film (Caro 2015 / Akiyama 2009, softened c33=260 GPa, eps_par=15) — high-coupling BAW/FBAR piezoelectric (kt^2 ~ 15-22%) vs stiffer lower-coupling aluminum_nitride.
APPROXIMATE 30% Sc-alloyed wurtzite Sc0.30Al0.70N compilation from M. A. Caro et al., J. Phys.: Condens. Matter 27, 245901 (2015) and M. Akiyama et al., Adv. Mater. 21, 593 (2009); film stoichiometry and stress strongly affect actual constants
silica amorphous isotropic
293.15 K
2201 kg/m^3
elasticthermaldielectricopticalphotoelasticviscoelastic
Fused silica glass (Corning HPFS 7980, E=72.7 GPa, Malitson 1965 Sellmeier 0.21-6.7 um, n=1.4440 at 1.55 um) — bulk baseline vs silica_thermal_box, silica_4k, and crystalline quartz_alpha.
Compiled from the per-table sources below. Density 2201 kg/m^3: Corning 7980 data sheet as reproduced by Abrisa Technologies (2.201 g/cm^3); Corning HPFS brochure gives 2.20 g/cm^3
silica_4k amorphous isotropic
4.0 K
2203 kg/m^3
elasticthermaldielectricopticalphotoelasticviscoelastic
Cryogenic fused silica SiO2 at 4 K (Fine 1954 / Hunklinger anomalous -4.5% glass softening E=70.0 GPa + TLS k=0.09 W/(m*K)) — softer glass mechanics and TLS thermal bottleneck vs 293 K silica.
APPROXIMATE 4 K fused silica mechanics/thermal/permittivity + inherited room-temperature Malitson [optical]; see M. E. Fine, H. Van Duyne, N. T. Kenney, J. Appl. Phys. 25, 402 (1954)
silica_thermal_box amorphous isotropic
293.15 K
2200 kg/m^3
elasticthermaldielectricopticalphotoelasticviscoelastic
Thermally grown SOI buried/pad oxide SiO2 (Hopcroft 2010 / MEMSCAP PADOXIDE, rho=2200 kg/m^3, E=70.0 GPa, nu=0.17, eps_r=3.9) — slightly softer wet/dry thin-film oxide vs bulk fused-quartz silica (E=72.7 GPa) and softened silica_4k.
Thermal and optical properties inherited from silica; density, [elastic] and [dielectric] set to MEMSCAP PiezoMUMPs / SOI buried-oxide thin-film values
silicon semiconductor m-3m
293.15 K
2329 kg/m^3
elasticthermaldielectricopticalphotoelasticviscoelasticnonlinearinterfaces
Single-crystal Si [100] at 293 K (Hopcroft 2010 cubic elastic + Li 1980 IR index 1.2-14 um, n=3.4757 at 1.55 um) — baseline vs silicon_salzberg, silicon_palik, silicon_mcskimin, silicon_4k.
Compiled from the per-table sources below. Density 2329 kg/m^3 (2.329 g/cm^3): El-Cat silicon properties page and Sydor/Ohara data sheet (2.33 g/cm^3), checked 2026-11-04
silicon_4k semiconductor m-3m
4.0 K
2330.5 kg/m^3
elasticthermaldielectricopticalinterfaces
Cryogenic high-resistivity FZ Si [100] at 4-10 K (McSkimin 1953 elastic c11=167.72 GPa + Franta/Frey 10 K index n=3.4488 at 1.55 um + Krupka eps_r=11.45) — ~1.3% stiffer and -0.027 lower n than 293 K silicon.
H. J. McSkimin, J. Appl. Phys. 24, 988-997 (1953) low-T elastic limit
silicon_mcskimin semiconductor m-3m
293.15 K
2329 kg/m^3
elasticthermaldielectricopticalphotoelasticviscoelasticnonlinearinterfaces
High-purity single-crystal Si [100] ultrasonic stiffness (McSkimin 1953, c11=165.7, c12=63.9, c44=79.6 GPa at 298 K) — acoustic pulse-echo reference vs Hopcroft 2010 MEMS silicon and cryogenic silicon_4k.
Density, thermal, electrical and optical properties inherited from silicon; [elastic] from H. J. McSkimin, J. Appl. Phys. 24, 988-997 (1953) at 298 K
silicon_nitride amorphous isotropic
293.15 K
3100 kg/m^3
elasticthermaldielectricopticalphotoelasticnonlinear
Stoichiometric LPCVD Si3N4 film at 293 K (Luke 2015 Sellmeier 0.31-5.5 um, n=1.9963 at 1.55 um; E=290 GPa) — low-loss photonic baseline vs UV-VIS silicon_nitride_philipp and higher-index silicon_nitride_pecvd.
APPROXIMATE thin-film compilation: [optical] verified from Luke et al. 2015; density 3100 kg/m^3 and mechanical/thermal/electrical are representative stoichiometric LPCVD Si3N4 film values that depend on furnace stress and stoichiometry
silicon_nitride_pecvd amorphous isotropic
293.15 K
2850 kg/m^3
elasticthermaldielectricoptical
Low-stress Si-rich PECVD SiNx film (Vogt 2015 ellipsometry 0.25-1.70 um, n=2.051 at 1.55 um, E=210 GPa) — higher-index 300 C CMOS-compatible film vs stoichiometric LPCVD silicon_nitride (n=1.9963, E=270 GPa).
APPROXIMATE PECVD SiNx density/mechanics/thermal/electrical + verified Vogt 2015 [optical] ellipsometry table (refractiveindex.info main/Si3N4/Vogt-2, CC0)
silicon_nitride_philipp amorphous isotropic
293.15 K
3100 kg/m^3
elasticthermaldielectricopticalphotoelasticnonlinear
Stoichiometric Si3N4 visible/NIR 1-term Sellmeier (Philipp 1973 / Baak 1982, 0.207-1.24 um, n=2.011 at 0.633 um) — classic visible-band fit vs Luke 2015 telecom/MIR silicon_nitride and Si-rich silicon_nitride_pecvd.
Mechanical, thermal and electrical properties inherited from silicon_nitride; [optical] from Philipp 1973 / Baak 1982 (refractiveindex.info main/Si3N4/Philipp, CC0)
silicon_palik semiconductor m-3m
293.15 K
2329 kg/m^3
elasticthermaldielectricopticalphotoelasticviscoelasticnonlinearinterfaces
Crystalline Si tabulated complex n,k (Palik 1985 / Aspnes & Studna 1983, 0.25-2.5 um) — captures UV/visible interband absorption k above 1.1 um bandgap unlike lossless IR silicon and silicon_salzberg.
Mechanical, thermal and electrical properties inherited from silicon; [optical] tabulated complex n,k from Palik Handbook of Optical Constants of Solids (Aspnes & Studna 1983 UV-NIR + Edwards NIR)
silicon_salzberg semiconductor m-3m
293.15 K
2329 kg/m^3
elasticthermaldielectricopticalphotoelasticviscoelasticnonlinearinterfaces
Float-zone Si NIR/MIR 3-term Sellmeier (Salzberg & Villa 1957, 1.36-11 um, n=3.4777 at 1.55 um) — classic refractiveindex.info fit (+0.0020 above Li 1980 baseline silicon; lossless vs silicon_palik).
Mechanical, thermal and electrical properties inherited from silicon; [optical] updated to Salzberg & Villa 1957 / Tatian 1984 Sellmeier fit (refractiveindex.info main/Si/Salzberg, CC0)
silver metal isotropic
293.15 K
10490 kg/m^3
elasticthermalelectricaloptical
Evaporated Ag wide-band Lorentz-Drude fit at 293 K (Rakic 1998, 0.25-12.4 um; E=83 GPa, sigma=6.30e7 S/m) — broadband analytical baseline vs sharper NIR experimental silver_johnson.
APPROXIMATE bulk polycrystalline mechanics/thermal/electrical + verified Rakic et al. 1998 [optical] fit (0.248-12.4 um)
silver_johnson metal isotropic
293.15 K
10490 kg/m^3
elasticthermalelectricaloptical
Evaporated Ag thin-film experimental n,k table (Johnson & Christy 1972, 0.188-1.937 um) — sharper low-loss NIR plasmonics table vs wide-band Rakic 1998 analytical Drude-Lorentz silver.
Mechanical, thermal and electrical properties inherited from silver; [optical] Johnson & Christy 1972 evaporated Ag table (refractiveindex.info main/Ag/Johnson, CC0)
tin superconductor
7265 kg/m^3
superconducting
White tin (beta-Sn) superconducting film (Tinkham 1996 / Kittel 2005: Tc=3.72 K, Delta_0=0.575 meV, lambda_L=34 nm, xi_0=230 nm, sigma_n=4.0e7 S/m) — compact BCS alias of beta_tin_sc.
Compiled from the per-table sources below. Density 7265 kg/m^3: C. Kittel, Introduction to Solid State Physics, 8th ed. (Wiley, 2005)
titanium_nitride_sc superconductor isotropic
0.02 K
5220 kg/m^3
elasticthermalsuperconductinginterfaces
Superconducting TiN thin film at <1 K (Leduc 2010 / Melville 2020: Tc=2.8-4.8 K, Lk=5-150 pH/sq, E=450 GPa) — ultra-high-Qi kinetic-inductance resonator/MKID nitride vs low-Lk aluminium_sc_emft.
APPROXIMATE superconducting TiN film compilation from H. G. Leduc et al., Appl. Phys. Lett. 97, 102509 (2010) & A. Melville et al., Appl. Phys. Lett. 117, 124004 (2020) + Kim et al. 1992